{"id":6030,"date":"2026-09-02T14:50:00","date_gmt":"2026-09-02T14:50:00","guid":{"rendered":"https:\/\/beiyutitanium.com\/?p=6030"},"modified":"2026-09-02T15:15:52","modified_gmt":"2026-09-02T15:15:52","slug":"titanium-seawater-velocity-erosion-limits","status":"publish","type":"post","link":"https:\/\/beiyutitanium.com\/de\/titanium-seawater-velocity-erosion-limits\/","title":{"rendered":"Titan in Meerwasser: Was die Daten zu Geschwindigkeit und Erosion tats\u00e4chlich zeigen"},"content":{"rendered":"<p>In den ver\u00f6ffentlichten TIMET-Tests zeigte unlegiertes Titan bei 25 ft\/sec (7.6 m\/sec) in sauberem Meerwasser keine messbare Erosion, und bei 120 ft\/sec (36.6 m\/sec) betrug die angegebene Rate 0.3 mpy (0.008 mm\/y). Dies sind Pr\u00fcfergebnisse unter den in der Quelle angegebenen Bedingungen, kein Auslegungsgrenzwert f\u00fcr Ihre Anlage. Was sie zeigen, ist, dass in sauberem Meerwasser nicht die Erosionsrate das begrenzende Element f\u00fcr ein Titanrohr ist. Zwei andere Dinge k\u00f6nnen es sein: schwebende Abrasivstoffe oberhalb einer bestimmten Beladung und Spaltbedingungen in hei\u00dfen konzentrierten Chloriden. Diese Seite gibt die ver\u00f6ffentlichten Zahlen f\u00fcr alle drei an, zusammen mit den Pr\u00fcfbedingungen.<\/p>\n<h2>Was zeigen die ver\u00f6ffentlichten Geschwindigkeitspr\u00fcfungen tats\u00e4chlich?<\/h2>\n<p>Drei Datenpunkte in sauberem Meerwasser f\u00fcr unlegiertes Titan und Ti-6Al-4V. Lesen Sie sie als das, was sie sind: Ergebnisse unter den angegebenen Bedingungen, nicht als zul\u00e4ssige Geschwindigkeit.<\/p>\n<div class=\"wp-block-table\" role=\"region\" tabindex=\"0\" aria-label=\"Erosionsdaten bei Meerwasser-Str\u00f6mungsgeschwindigkeit\" style=\"overflow-x:auto;-webkit-overflow-scrolling:touch;max-width:100%;\">\n<table style=\"min-width:780px;\">\n<caption>Erosion von unlegiertem Titan und Ti-6Al-4V in Meerwasser, gem\u00e4\u00df dem ver\u00f6ffentlichten TIMET-Handbuch zur Korrosionsbest\u00e4ndigkeit von Titan.<\/caption>\n<thead>\n<tr>\n<th>Str\u00f6mungsgeschwindigkeit in Meerwasser<\/th>\n<th>Erosionsrate von unlegiertem Titan<\/th>\n<th>Ti-6Al-4V<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>0 to 2 ft\/sec (0 to 0,61 m\/sec)<\/td>\n<td>Null<\/td>\n<td>Nicht angegeben<\/td>\n<\/tr>\n<tr>\n<td>25 ft\/sec (7,6 m\/sec)<\/td>\n<td>Null<\/td>\n<td>Nicht angegeben<\/td>\n<\/tr>\n<tr>\n<td>120 ft\/sec (36,6 m\/sec)<\/td>\n<td>0.3 mpy (0.008 mm\/y)<\/td>\n<td>0.4 mpy (0.010 mm\/y)<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p>Werte aus dem ver\u00f6ffentlichten Titan-Korrosionsbest\u00e4ndigkeitshandbuch von TIMET (Titanium Metals Corporation), Erosion von unlegiertem Titan und Ti-6Al-4V in Meerwasser. Zwei Grenzen, wie weit dies tr\u00e4gt. \u201eNil\u201c bedeutet keinen mit der Quellmethode messbaren Verlust, nicht null. Und die Quelle gibt f\u00fcr diese Zeilen weder die Pr\u00fcfgeometrie, ob die angegebene Geschwindigkeit Massenstr\u00f6mung oder lokaler Aufprall ist, die Wasserchemie noch die Expositionsdauer an, sodass die Zahlen das Material einordnen, statt eine Rohrkonfiguration zu qualifizieren. Ihre eigene Auslegungsgeschwindigkeit muss weiterhin gegen Aufprall an Einl\u00e4ufen und B\u00f6gen sowie gegen str\u00f6mungsinduzierte Schwingungen gepr\u00fcft werden.<\/p>\n<h2>Wo Titan tats\u00e4chlich verliert: Abrasivstoffbeladung<\/h2>\n<p>In sauberem Wasser bleibt die Erosionsrate \u00fcber die gepr\u00fcften Geschwindigkeiten niedrig, entscheidend ist jedoch, was das Wasser mitf\u00fchrt. Dieselbe ver\u00f6ffentlichte Quelle berichtet \u00fcber Pr\u00fcfungen mit abrasiven Zus\u00e4tzen von 6.6 bis 23.6 ft\/sec, mit 2000 Stunden bei Sandbeladungen realer Wasserentnahmen und mit nur 1 Stunde bei Suspensionsbeladungen. Die Geschwindigkeit ist weiterhin wichtig, ebenso Partikelgr\u00f6\u00dfe, H\u00e4rte und Auftreffwinkel; die nachstehenden Zeilen variieren mehr als einen Faktor gleichzeitig und sollten als Screening-Ergebnisse gelesen werden:<\/p>\n<div class=\"wp-block-table\" role=\"region\" tabindex=\"0\" aria-label=\"Erosionsdaten bei Schwebstoffen\" style=\"overflow-x:auto;-webkit-overflow-scrolling:touch;max-width:100%;\">\n<table style=\"min-width:980px;\">\n<caption>Erosion in Meerwasser mit Schwebstoffen, gem\u00e4\u00df dem ver\u00f6ffentlichten TIMET-Handbuch zur Korrosionsbest\u00e4ndigkeit von Titan.<\/caption>\n<thead>\n<tr>\n<th>Zustand<\/th>\n<th>Unlegiertes Titan<\/th>\n<th>70Cu-30Ni<\/th>\n<th>Aluminiummessing<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Sauberes Meerwasser, 23.6 ft\/sec, 10000 h<\/td>\n<td>Null<\/td>\n<td>Lochfra\u00df<\/td>\n<td>Lochfra\u00df<\/td>\n<\/tr>\n<tr>\n<td>40 g\/l 60-mesh-Sand, 6.6 ft\/sec, 2000 h<\/td>\n<td>0.1 mpy (0.0025 mm\/y)<\/td>\n<td>3.9 mpy (0.10 mm\/y)<\/td>\n<td>2.0 mpy (0.05 mm\/y)<\/td>\n<\/tr>\n<tr>\n<td>40 g\/l 10-mesh-Schmirgel, 6.6 ft\/sec, 2000 h<\/td>\n<td>0.5 mpy (0.0125 mm\/y)<\/td>\n<td>Starke Erosion<\/td>\n<td>Starke Erosion<\/td>\n<\/tr>\n<tr>\n<td>4 Prozent 80-mesh-Schmirgel, 13.5 ft\/sec, 17.5 h<\/td>\n<td>3.3 mpy (0.083 mm\/y)<\/td>\n<td>2.6 mpy (0.065 mm\/y)<\/td>\n<td>Nicht angegeben<\/td>\n<\/tr>\n<tr>\n<td>40 Prozent 80-mesh-Schmirgel, 23.6 ft\/sec, 1 h<\/td>\n<td>59.1 mpy (1.5 mm\/y)<\/td>\n<td>78.7 mpy (2.0 mm\/y)<\/td>\n<td>Nicht angegeben<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p>Lesen Sie die letzten zwei Zeilen sorgf\u00e4ltig, denn sie sind der ehrliche Teil. Bei 4 Prozent Schmirgelbeladung ist das Kupfernickel marginal besser als Titan, und bei 40 Prozent Beladung liegen beide Raten \u00fcber 1 mm pro Jahr. Beachten Sie, was die letzte Zeile ist: eine 1-Stunden-Pr\u00fcfung mit auf eine Jahresrate hochgerechneter Abtragung. Das ist eine Screening-Zahl, keine Einsatzrate, und die Spalte f\u00fcr Aluminium-Messing ist f\u00fcr keine dieser beiden Zeilen angegeben, sodass die Einordnung dort unvollst\u00e4ndig ist. Titan ist kein abriebfestes Material; bei den Sandbeladungen, die eine reale Wasserentnahme aufweist, ist es deutlich besser, und es ist nicht mehr die L\u00f6sung, wenn das Medium faktisch eine Suspension ist. Werte aus demselben TIMET-Handbuch, Erosion von unlegiertem Titan in Meerwasser mit suspendierten Feststoffen.<\/p>\n<h2>Was Langzeitexpositionen an realen Standorten zeigen<\/h2>\n<div class=\"wp-block-table\" role=\"region\" tabindex=\"0\" aria-label=\"Meerwasser-Erosionsdaten benannter Standorte\" style=\"overflow-x:auto;-webkit-overflow-scrolling:touch;max-width:100%;\">\n<table style=\"min-width:760px;\">\n<caption>Erosion an genannten Meerwasserstandorten, gem\u00e4\u00df dem ver\u00f6ffentlichten TIMET-Handbuch zur Korrosionsbest\u00e4ndigkeit von Titan.<\/caption>\n<thead>\n<tr>\n<th>Ort und Str\u00f6mung<\/th>\n<th>Dauer<\/th>\n<th>Unlegiertes Titan<\/th>\n<th>70Cu-30Ni<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Brixham Sea, 32.2 ft\/sec (9.8 m\/sec)<\/td>\n<td>12 Monate<\/td>\n<td>Unter 0.098 mpy (unter 0.0025 mm\/y)<\/td>\n<td>11.8 mpy (0.3 mm\/y)<\/td>\n<\/tr>\n<tr>\n<td>Kure Beach, 3.3 ft\/sec (1 m\/sec)<\/td>\n<td>54 Monate<\/td>\n<td>0.00003 mpy (0.00000075 mm\/y)<\/td>\n<td>Nicht angegeben<\/td>\n<\/tr>\n<tr>\n<td>Wrightsville Beach, 2.0 bis 4.3 ft\/sec<\/td>\n<td>6 Monate<\/td>\n<td>0.004 mpy (0.0001 mm\/y)<\/td>\n<td>0.9 mpy (0.022 mm\/y)<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p>Bei Brixham wurde die Aluminiumprobe im selben Test durchl\u00f6chert. Dies sind mehrmonatige und mehrj\u00e4hrige Expositionen an benannten Standorten, keine Laborstunden, weshalb sie in einer Auslegungspr\u00fcfung mehr Gewicht haben als ein einzelner beschleunigter Test.<\/p>\n<h2>Der Grenzwert, der tats\u00e4chlich \u00fcber Ihr Grade entscheidet: Spaltkorrosion<\/h2>\n<p>Die Geschwindigkeit bestimmt die Titang\u00fcte nur selten. Hei\u00dfe konzentrierte Chloride in einem Spalt tun dies. Die ver\u00f6ffentlichten 500-Stunden-Siedepr\u00fcfungen mit Metall-zu-PTFE-Spaltproben unterscheiden die G\u00fcten eindeutig:<\/p>\n<div class=\"wp-block-table\" role=\"region\" tabindex=\"0\" aria-label=\"G\u00fctevergleich bei siedender Spaltkorrosion\" style=\"overflow-x:auto;-webkit-overflow-scrolling:touch;max-width:100%;\">\n<table style=\"min-width:980px;\">\n<caption>Best\u00e4ndigkeit gegen Spaltkorrosion in siedenden L\u00f6sungen, 500-Stunden-Tests mit Metall-PTFE-Spaltproben, gem\u00e4\u00df dem ver\u00f6ffentlichten TIMET-Handbuch zur Korrosionsbest\u00e4ndigkeit von Titan.<\/caption>\n<thead>\n<tr>\n<th>Siedende Umgebung<\/th>\n<th>pH<\/th>\n<th>Unlegiert (Grade-2-Klasse)<\/th>\n<th>Ti-0.3Mo-0.8Ni (Grade 12)<\/th>\n<th>Palladiumhaltig (Grade-7-Klasse)<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Ges\u00e4ttigtes NaCl<\/td>\n<td>3.0<\/td>\n<td>Versagt<\/td>\n<td>Best\u00e4ndig<\/td>\n<td>Best\u00e4ndig<\/td>\n<\/tr>\n<tr>\n<td>Ges\u00e4ttigtes ZnCl2<\/td>\n<td>3.0<\/td>\n<td>Versagt<\/td>\n<td>Best\u00e4ndig<\/td>\n<td>Best\u00e4ndig<\/td>\n<\/tr>\n<tr>\n<td>42 Prozent MgCl2<\/td>\n<td>4.2<\/td>\n<td>Versagt<\/td>\n<td>Best\u00e4ndig<\/td>\n<td>Best\u00e4ndig<\/td>\n<\/tr>\n<tr>\n<td>10 Prozent NH4Cl<\/td>\n<td>4.1<\/td>\n<td>Versagt<\/td>\n<td>Best\u00e4ndig<\/td>\n<td>Best\u00e4ndig<\/td>\n<\/tr>\n<tr>\n<td>10 Prozent Na2SO4<\/td>\n<td>2.0<\/td>\n<td>Versagt<\/td>\n<td>Best\u00e4ndig<\/td>\n<td>Best\u00e4ndig<\/td>\n<\/tr>\n<tr>\n<td>Ges\u00e4ttigtes NaCl plus Cl2<\/td>\n<td>2.0<\/td>\n<td>Versagt<\/td>\n<td>Versagt<\/td>\n<td>Best\u00e4ndig<\/td>\n<\/tr>\n<tr>\n<td>10 Prozent FeCl3<\/td>\n<td>0.6<\/td>\n<td>Versagt<\/td>\n<td>Versagt<\/td>\n<td>Best\u00e4ndig<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p>Was diese Tabelle eng gefasst belegt: \u00dcber diese sieben siedenden L\u00f6sungen mit engem Spalt hinweg versagte das unlegierte Grade in allen, Grade 12 hielt in f\u00fcnf und versagte in den beiden oxidierenden Chloridumgebungen, und das palladiumhaltige Grade hielt in allen sieben. Das ist eine Grade-Rangfolge unter einer schweren Screening-Bedingung. Es ist keine Einsatzgrenze, da die Tabelle keinen Temperaturbereich unterhalb des Siedepunkts, keine Chloridaktivit\u00e4t, keine andere Spaltgeometrie als die verwendete, keine W\u00e4rme\u00fcbertragungsbedingung und keine zul\u00e4ssige Angriffstiefe enth\u00e4lt. Verwenden Sie sie, um die Rangfolge der Grades zu kennen und zu wissen, dass oxidierende Chloride Grade 12 vom Palladium-Grade trennen; verwenden Sie Ihre eigenen Einsatzdaten, um den tats\u00e4chlichen Betrieb einzuordnen. Meerwasser bei Umgebungstemperatur ist \u00fcberhaupt nicht diese Umgebung, und unlegiertes Titan ist dort die richtige und normale Wahl.<\/p>\n<h2>Die Variable, die diese Seite nicht kl\u00e4rt: Temperatur<\/h2>\n<p>Die obigen Tests sind entweder Meerwasser bei Umgebungstemperatur oder siedend. Der gr\u00f6\u00dfte Teil des realen Betriebs liegt zwischen beiden, und in dieser L\u00fccke wird die Grade-Wahl tats\u00e4chlich entschieden. Dasselbe TIMET-Handbuch gibt eine allgemeine Meerwasser-Korrosionsbest\u00e4ndigkeit bis zu Temperaturen von 500 F (260 C) an und bildet die Spaltkorrosionsgrenze f\u00fcr jeden Grade als Funktion von Temperatur und pH-Wert in ges\u00e4ttigter NaCl-Sole ab. Wenn Ihr Einsatzfall ein chlorierter Meerwasserkreislauf bei 60 C ist, beantworten weder die Daten bei Umgebungstemperatur noch die Siededaten dies; die Temperatur-pH-Karte tut es. Senden Sie die Betriebstemperatur, den pH-Wert und den Chlorrestgehalt mit der Anfrage, und der Betrieb kann anhand dieser Grenze eingeordnet werden, statt aus den beiden Extremen dieser Seite gesch\u00e4tzt zu werden.<\/p>\n<h2>Wo Titan komplett die falsche Antwort ist<\/h2>\n<div class=\"wp-block-table\" role=\"region\" tabindex=\"0\" aria-label=\"Bedingungen, die Titan ausschlie\u00dfen\" style=\"overflow-x:auto;-webkit-overflow-scrolling:touch;max-width:100%;\">\n<table style=\"min-width:700px;\">\n<thead>\n<tr>\n<th>Zustand<\/th>\n<th>Warum Titan ausgeschlossen ist<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>Fluorgas sowie Fluoride in saurem w\u00e4ssrigem Einsatz<\/td>\n<td>Flusss\u00e4ure kann sich aus kleinsten Mengen bilden und greift Titan rasch an; die ver\u00f6ffentlichte Anleitung besagt ausdr\u00fccklich, dass Titan bei Kontakt mit Fluorgas nicht empfohlen wird<\/td>\n<\/tr>\n<tr>\n<td>Abrasivstoffbeladung im Schlammbereich<\/td>\n<td>Siehe die 40-Prozent-Schmirgel-Zeile oben: sowohl Titan als auch Kupfer-Nickel versagen<\/td>\n<\/tr>\n<tr>\n<td>Trockenes Chlor oder trockenes Brom<\/td>\n<td>Titan wird durch das trockene Gas angegriffen und durch die Anwesenheit von Feuchtigkeit passiviert<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p>Die Angabe der Ausschl\u00fcsse ist Teil einer verwendbaren Auswahlseite. Ein Lieferant, der nur auflistet, was ein Metall \u00fcbersteht, hat Ihnen nicht genug f\u00fcr die Auslegung gegeben.<\/p>\n<h2>Was dies f\u00fcr die Bestellung bedeutet<\/h2>\n<div class=\"wp-block-table\" role=\"region\" tabindex=\"0\" aria-label=\"Anfrageanforderungen f\u00fcr Titan im Meerwassereinsatz\" style=\"overflow-x:auto;-webkit-overflow-scrolling:touch;max-width:100%;\">\n<table style=\"min-width:780px;\">\n<thead>\n<tr>\n<th>Bestellposition<\/th>\n<th>Was anzugeben ist<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>G\u00fcte und Norm<\/td>\n<td>Grade 2 nach ASTM B338 f\u00fcr Meerwasserrohr bei Umgebungstemperatur; Grade 12 oder Grade 7, wo hei\u00dfe Chlorid-Spaltbedingungen plausibel sind<\/td>\n<\/tr>\n<tr>\n<td>Mitzuteilende Einsatzdaten<\/td>\n<td>Medium, Chloridkonzentration, Temperatur, pH-Wert, Dosierung von freiem Chlor und erwartete Schwebstoffe<\/td>\n<\/tr>\n<tr>\n<td>Geschwindigkeit<\/td>\n<td>Geben Sie die Auslegungsgeschwindigkeit an, damit Wanddicke und St\u00fctzabstand gegen\u00fcber Schwingung gepr\u00fcft werden, nicht gegen\u00fcber Erosion<\/td>\n<\/tr>\n<tr>\n<td>Pr\u00fcfung<\/td>\n<td>Geben Sie die Ultraschall-Abnahmeklasse und die Verfahrensnorm f\u00fcr das Rohr sowie etwaige Anforderungen an die Wirbelstrompr\u00fcfung an<\/td>\n<\/tr>\n<tr>\n<td>Zertifikat<\/td>\n<td>EN 10204 Typ 3.1 mit Chargen- und Schmelznummern<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p>Eine Folge, die es klar zu benennen lohnt, weil sie eine Zeichnung \u00e4ndert: In sauberem str\u00f6mendem Meerwasser sind die ver\u00f6ffentlichten Erosionsraten niedrig genug, dass Titanrohr normalerweise nach Druck und Schwingung ausgelegt wird und nicht nach einer Korrosionszugabe an der Wand. Ein praktischer Hinweis aus der Angebotserstellung f\u00fcr diese Arbeit: Bei Titan-Meerwasserrohr sind \u00fcblicherweise die str\u00f6mungsinduzierte Schwingung und der St\u00fctzabstand die ma\u00dfgeblichen Auslegungsgrenzen, nicht der Materialabtrag. Das \u00e4ndert, was Ihre Anfrage von uns best\u00e4tigt haben sollte.<\/p>\n<h2>Spezifikationsdetails mit Quellenangabe<\/h2>\n<p>Die obigen Korrosions- und Erosionswerte stammen aus dem ver\u00f6ffentlichten Handbuch zur Korrosionsbest\u00e4ndigkeit von Titan von TIMET (Titanium Metals Corporation): Erosion von unlegiertem Titan und Ti-6Al-4V in Meerwasser bei 0 bis 2, 25 und 120 ft\/sec; Erosion in Meerwasser mit Schwebstoffen bei den angegebenen Abrasivstoffbeladungen und Dauern; Erosion an genannten Meerwasserstandorten \u00fcber 6 bis 54 Monate; sowie Best\u00e4ndigkeit gegen Spaltkorrosion in siedenden L\u00f6sungen aus 500-Stunden-Tests mit Metall-PTFE-Spaltproben. Grade-Identit\u00e4ten und Grenzwerte gelten nach ASTM B338 f\u00fcr nahtloses und geschwei\u00dftes Rohr; die hier angegebenen Zusammensetzungswerte sind die entsprechenden Grade-Identit\u00e4ten, wobei ASTM B348 nur zitiert wird, wo Stab die Produktform ist. Grade 2 unter UNS R50400 mit Sauerstoff bei maximal 0,25 Prozent und Zugfestigkeit bei mindestens 345 MPa im gegl\u00fchten Zustand, Grade 7 unter UNS R52400 mit Palladium bei 0,12 bis 0,25 Prozent, und Grade 12 unter UNS R53400 mit Molybd\u00e4n bei 0,2 bis 0,4 Prozent und Nickel bei 0,6 bis 0,9 Prozent.<\/p>\n<p>Hinweis zum Anwendungsbereich der Spaltdaten: Diese Ergebnisse beschreiben siedende konzentrierte L\u00f6sungen mit einem absichtlich engen Metall-PTFE-Spalt \u00fcber 500 Stunden. Es handelt sich um einen Grade-Rangfolgetest, keine Vorhersage der Einsatzdauer in Ihrer Anlage, und sie beschreiben nicht Meerwasser bei Umgebungstemperatur, wo unlegiertes Titan die normale Wahl ist. Beiyu Titanium liefert das Rohr und den Stab nach den oben genannten Normen mit einem Abnahmepr\u00fcfzeugnis 3.1 nach EN 10204 gem\u00e4\u00df dem Bestellumfang; die Korrosionsdaten sind ver\u00f6ffentlichte Pr\u00fcfdaten Dritter, keine Pr\u00fcfergebnisse von Beiyu.<\/p>\n<h2>H\u00e4ufig gestellte Fragen<\/h2>\n<p><strong>Gibt es eine maximale Meerwassergeschwindigkeit f\u00fcr Kondensatorrohr aus Titan?<\/strong> Die ver\u00f6ffentlichten Daten geben keinen an. TIMET gibt 0.3 mpy (0.008 mm\/y) bei 120 ft\/sec (36.6 m\/sec) in sauberem Meerwasser an, was zeigt, dass Erosion nicht die erste Einschr\u00e4nkung ist, aber die Quelle gibt weder die Pr\u00fcfgeometrie an noch, ob diese Geschwindigkeit eine Grundstr\u00f6mung oder ein Auftreffen ist. In der Praxis stammen die ma\u00dfgeblichen Grenzwerte aus str\u00f6mungsinduzierter Schwingung, St\u00fctzabstand und Einlassauftreffen, was mechanische Auslegungsfragen sind und in Ihre Rohrauslegungsgrundlage geh\u00f6ren, nicht in eine Korrosionstabelle.<\/p>\n<p><strong>\u00c4ndert Sand im Ansaugstrom die Antwort?<\/strong> Im selben TIMET-Handbuch lief unlegiertes Titan bei 40 g\/l 60-mesh-Sand und 6.6 ft\/sec \u00fcber 2000 Stunden mit 0.1 mpy, w\u00e4hrend 70Cu-30Ni im selben Test 3.9 mpy erreichte. Titan ist bei realen Ansaugbeladungen deutlich besser. Bei Schlammbeladungen versagen beide Materialien, und die ehrliche Antwort dort ist, dass keines von beiden die richtige Wahl ist.<\/p>\n<p><strong>Wann muss ich von Grade 2 abweichen?<\/strong> Wenn sich hei\u00dfe konzentrierte Chloride in einem Spalt festsetzen k\u00f6nnen. Grade 12 deckt den gr\u00f6\u00dften Teil dieses Bereichs ab; freies Chlor oder Eisen(III)-chlorid verschiebt die Wahl zum palladiumhaltigen Grade. Der Mechanismus und die Grade-Logik stehen in <a href=\"https:\/\/beiyutitanium.com\/de\/grade-12-titanium-hot-brine-crevice-corrosion\/\">Grade-12-Titan in hei\u00dfer Sole und Spalteinsatz<\/a> und <a href=\"https:\/\/beiyutitanium.com\/de\/grade-7-titanium-reducing-acids\/\">Titan Grade 7 in reduzierenden S\u00e4uren<\/a>.<\/p>\n<p><strong>Wie schneidet Titan im Vergleich zu Kupfer-Nickel insgesamt f\u00fcr Meerwasser ab?<\/strong> Der Werkstoffvergleich \u00fcber den Meerwassereinsatz hinweg steht in <a href=\"https:\/\/beiyutitanium.com\/de\/titanium-vs-stainless-vs-copper-nickel-seawater\/\">Titan im Vergleich zu Edelstahl und Kupfer-Nickel in Meerwasser<\/a>.<\/p>\n<p><strong>Welche Rohrnorm gilt?<\/strong> ASTM B338 erfasst nahtloses und geschwei\u00dftes Titanrohr f\u00fcr Kondensatoren und W\u00e4rmetauscher; der Leitfaden steht unter <a href=\"https:\/\/beiyutitanium.com\/de\/astm-b338-titanium-tube-pipe-guide\/\">dem Leitfaden zu ASTM B338 Titanrohr<\/a>.<\/p>\n<h2>Senden Sie die Einsatzdaten mit der Anfrage<\/h2>\n<p>Senden Sie Medium, Chloridkonzentration, Temperatur, pH-Wert, Chlordosierung, Schwebstoffe und Auslegungsgeschwindigkeit zusammen mit dem Grade, der Norm, Abmessungen und Menge an <a href=\"https:\/\/beiyutitanium.com\/de\/contact\/\">die Beiyu-RFQ-Seite<\/a>. Gepr\u00fcft von <a href=\"https:\/\/beiyutitanium.com\/de\/penn-ma\/\">Penn Ma<\/a>, 15 Jahre im Titan-Halbzeug-Export. Zuletzt \u00fcberpr\u00fcft: 2026-09-01.<\/p>","protected":false},"excerpt":{"rendered":"<p>In the published TIMET tests, unalloyed titanium showed no measurable erosion in clean seawater at 25 ft\/sec (7.6 m\/sec), and at 120 ft\/sec (36.6 m\/sec) the reported rate was 0.3 mpy (0.008 mm\/y). Those are test results at the conditions the source states, not a design limit for your equipment. What they do show is [&hellip;]<\/p>\n","protected":false},"author":2,"featured_media":0,"comment_status":"closed","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"_templately_pack_id":"","_templately_imported_at":"","_templately_source":"","_templately_import_session_id":"","site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"default","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","ast-disable-related-posts":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-4)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-4)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-4)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"categories":[27,137],"tags":[],"class_list":["post-6030","post","type-post","status-publish","format-standard","hentry","category-news","category-technical-guides"],"yoast_head":"<!-- This site is optimized with the Yoast SEO plugin v28.6 - https:\/\/yoast.com\/product\/yoast-seo-wordpress\/ -->\n<title>Titanium Seawater Velocity and Erosion Limits: The Published Data | Beiyu<\/title>\n<meta name=\"description\" content=\"Published erosion rates for titanium in seawater at 25 and 120 ft\/sec, with suspended solids, and 500-hour crevice results by grade. Test conditions stated, failure boundaries included.\" \/>\n<meta name=\"robots\" content=\"index, follow, max-snippet:-1, max-image-preview:large, max-video-preview:-1\" \/>\n<link rel=\"canonical\" href=\"https:\/\/beiyutitanium.com\/de\/titanium-seawater-velocity-erosion-limits\/\" \/>\n<meta property=\"og:locale\" content=\"de_DE\" \/>\n<meta property=\"og:type\" content=\"article\" \/>\n<meta property=\"og:title\" content=\"Titanium Seawater Velocity and Erosion Limits: The Published Data | Beiyu\" \/>\n<meta property=\"og:description\" content=\"Published erosion rates for titanium in seawater at 25 and 120 ft\/sec, with suspended solids, and 500-hour crevice results by grade. Test conditions stated, failure boundaries included.\" \/>\n<meta property=\"og:url\" content=\"https:\/\/beiyutitanium.com\/de\/titanium-seawater-velocity-erosion-limits\/\" \/>\n<meta property=\"og:site_name\" content=\"Beiyu Titanium\" \/>\n<meta property=\"article:published_time\" content=\"2026-09-02T14:50:00+00:00\" \/>\n<meta property=\"article:modified_time\" content=\"2026-09-02T15:15:52+00:00\" \/>\n<meta property=\"og:image\" content=\"https:\/\/beiyutitanium.com\/wp-content\/uploads\/2026\/06\/grade-12-titanium-weld-neck-flange-astm-b381-asme-b16-5-scaled.jpg\" \/>\n\t<meta property=\"og:image:width\" content=\"1200\" \/>\n\t<meta property=\"og:image:height\" content=\"999\" \/>\n\t<meta property=\"og:image:type\" content=\"image\/jpeg\" \/>\n<meta name=\"author\" content=\"Penn Ma\" \/>\n<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n<meta name=\"twitter:label1\" content=\"Written by\" \/>\n\t<meta name=\"twitter:data1\" content=\"Penn Ma\" \/>\n\t<meta name=\"twitter:label2\" content=\"Est. reading time\" \/>\n\t<meta name=\"twitter:data2\" content=\"9 minutes\" \/>\n<script type=\"application\/ld+json\" class=\"yoast-schema-graph\">{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"Article\",\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/titanium-seawater-velocity-erosion-limits\\\/#article\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/titanium-seawater-velocity-erosion-limits\\\/\"},\"author\":{\"name\":\"Penn Ma\",\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/#\\\/schema\\\/person\\\/3560db17cf08813edf34f012735b971b\"},\"headline\":\"Titanium in Seawater: What the Velocity and Erosion Data Actually Show\",\"datePublished\":\"2026-09-02T14:50:00+00:00\",\"dateModified\":\"2026-09-02T15:15:52+00:00\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/titanium-seawater-velocity-erosion-limits\\\/\"},\"wordCount\":1884,\"publisher\":{\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/#organization\"},\"articleSection\":[\"News\",\"Technical Guides\"],\"inLanguage\":\"de-DE\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/titanium-seawater-velocity-erosion-limits\\\/\",\"url\":\"https:\\\/\\\/beiyutitanium.com\\\/titanium-seawater-velocity-erosion-limits\\\/\",\"name\":\"Titanium Seawater Velocity and Erosion Limits: The Published Data | Beiyu\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/#website\"},\"datePublished\":\"2026-09-02T14:50:00+00:00\",\"dateModified\":\"2026-09-02T15:15:52+00:00\",\"description\":\"Published erosion rates for titanium in seawater at 25 and 120 ft\\\/sec, with suspended solids, and 500-hour crevice results by grade. Test conditions stated, failure boundaries included.\",\"breadcrumb\":{\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/titanium-seawater-velocity-erosion-limits\\\/#breadcrumb\"},\"inLanguage\":\"de-DE\",\"potentialAction\":[{\"@type\":\"ReadAction\",\"target\":[\"https:\\\/\\\/beiyutitanium.com\\\/titanium-seawater-velocity-erosion-limits\\\/\"]}]},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/titanium-seawater-velocity-erosion-limits\\\/#breadcrumb\",\"itemListElement\":[{\"@type\":\"ListItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/beiyutitanium.com\\\/\"},{\"@type\":\"ListItem\",\"position\":2,\"name\":\"Titanium in Seawater: What the Velocity and Erosion Data Actually Show\"}]},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/#website\",\"url\":\"https:\\\/\\\/beiyutitanium.com\\\/\",\"name\":\"Beiyu Titanium\",\"description\":\"Certified titanium materials and custom components for aerospace, medical, chemical, and industrial applications.\",\"publisher\":{\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/#organization\"},\"potentialAction\":[{\"@type\":\"SearchAction\",\"target\":{\"@type\":\"EntryPoint\",\"urlTemplate\":\"https:\\\/\\\/beiyutitanium.com\\\/?s={search_term_string}\"},\"query-input\":{\"@type\":\"PropertyValueSpecification\",\"valueRequired\":true,\"valueName\":\"search_term_string\"}}],\"inLanguage\":\"de-DE\"},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/#organization\",\"name\":\"Beiyu Titanium\",\"alternateName\":\"\u5317\u9a6d\u949b\u4e1a\",\"url\":\"https:\\\/\\\/beiyutitanium.com\\\/\",\"logo\":{\"@type\":\"ImageObject\",\"inLanguage\":\"de-DE\",\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/#\\\/schema\\\/logo\\\/image\\\/\",\"url\":\"https:\\\/\\\/beiyutitanium.com\\\/wp-content\\\/uploads\\\/2026\\\/03\\\/logo4.png\",\"contentUrl\":\"https:\\\/\\\/beiyutitanium.com\\\/wp-content\\\/uploads\\\/2026\\\/03\\\/logo4.png\",\"width\":429,\"height\":116,\"caption\":\"Beiyu Titanium\"},\"image\":{\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/#\\\/schema\\\/logo\\\/image\\\/\"},\"sameAs\":[\"https:\\\/\\\/www.linkedin.com\\\/company\\\/113015050\\\/\",\"https:\\\/\\\/www.youtube.com\\\/channel\\\/UC4Rr5qjUmKbbnROzU8zwluQ\",\"https:\\\/\\\/www.instagram.com\\\/beiyutrade\\\/\",\"https:\\\/\\\/www.facebook.com\\\/people\\\/Beiyu-Titanium-Group\\\/61580787646046\\\/\",\"https:\\\/\\\/www.crunchbase.com\\\/organization\\\/beiyu-titanium\",\"https:\\\/\\\/www.wikidata.org\\\/wiki\\\/Q140386451\"],\"contactPoint\":{\"@type\":\"ContactPoint\",\"contactType\":\"sales\",\"email\":\"penn@beiyutitanium.com\",\"availableLanguage\":[\"English\",\"Chinese\"]},\"description\":\"Beiyu Titanium (legal entity Jiaxing Beiyu New Materials Technology Co., Ltd.) is a China-based supplier and exporter of ASTM and AMS titanium bar, plate, sheet, tube, pipe, forgings, flanges, fasteners and custom machined parts, plus nickel and Inconel alloys, for chemical, marine, medical and industrial buyers worldwide. Production runs through the Beiyu titanium mill in Baoji, Shaanxi. Orders are RFQ-based, with EN 10204 3.1 mill test certificates and heat-number traceability available on request.\",\"areaServed\":\"Worldwide\",\"knowsAbout\":[\"Titanium\",\"Titanium alloy\",\"Titanium bar\",\"Titanium sheet and plate\",\"Titanium tube and pipe\",\"Titanium forgings\",\"Titanium wire\",\"Titanium anode\"],\"address\":{\"@type\":\"PostalAddress\",\"streetAddress\":\"Baotai Road Industrial Park, High-tech Development Zone\",\"addressLocality\":\"Baoji\",\"addressRegion\":\"Shaanxi\",\"addressCountry\":\"CN\"},\"legalName\":\"Jiaxing Beiyu New Materials Technology Co., Ltd.\"},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/beiyutitanium.com\\\/#\\\/schema\\\/person\\\/3560db17cf08813edf34f012735b971b\",\"name\":\"Penn Ma\",\"image\":{\"@type\":\"ImageObject\",\"inLanguage\":\"de-DE\",\"@id\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/0659bdefb633d0d8e567b06d2f8bffac2a369834e53e96c922a06fd8a96f3c72?s=96&d=mm&r=g\",\"url\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/0659bdefb633d0d8e567b06d2f8bffac2a369834e53e96c922a06fd8a96f3c72?s=96&d=mm&r=g\",\"contentUrl\":\"https:\\\/\\\/secure.gravatar.com\\\/avatar\\\/0659bdefb633d0d8e567b06d2f8bffac2a369834e53e96c922a06fd8a96f3c72?s=96&d=mm&r=g\",\"caption\":\"Penn Ma\"},\"description\":\"Penn Ma is the person who answers the RFQs at Beiyu Titanium. Over 15 years in titanium export he has learned to review each specification line himself, checking grade, standard, dimensions, tolerance and certificate scope against mill capability before quoting, rather than routing enquiries through a sales desk. He came to titanium supply from the other side of the transaction. Before leading Beiyu's international business he worked at Koch (Koch-Glitsch) and was directly involved in delivering a SABIC petrochemical project in Fujian, China. That work was built on inspection and test plans, material certification and heat traceability, third party inspection coordination, and project documentation and dossier control. Those are the same four things a process industry or regulated buyer will hold a titanium supplier to, and having had to enforce them as a customer is why they are treated here as part of the supply rather than as paperwork produced afterwards. His day-to-day work spans the questions this site is written to answer: choosing between commercially pure and alloyed titanium grades for a corrosive service, reading a mill test certificate against the ordered standard, and matching a buyer's designation (ASTM grade, UNS, German Werkstoff number or French NF code) to the same metal across markets. Beiyu supplies titanium, nickel-alloy and refractory mill products across bar, rod, plate, tube, block, ring, coil, ingot, forgings and machined parts, with EN 10204 3.1 documentation and heat-number traceability.\",\"url\":\"https:\\\/\\\/beiyutitanium.com\\\/de\\\/author\\\/penn-ma\\\/\"}]}<\/script>\n<!-- \/ Yoast SEO plugin. -->","yoast_head_json":{"title":"Grenzwerte f\u00fcr Titan im Meerwasser bei Str\u00f6mungsgeschwindigkeit und Erosion: Die ver\u00f6ffentlichten Daten | Beiyu","description":"Ver\u00f6ffentlichte Erosionsraten f\u00fcr Titan in Meerwasser bei 25 und 120 ft\/sec, mit Schwebstoffen, sowie 500-Stunden-Spaltkorrosionsergebnisse nach G\u00fcte. Pr\u00fcfbedingungen angegeben, Versagensgrenzen enthalten.","robots":{"index":"index","follow":"follow","max-snippet":"max-snippet:-1","max-image-preview":"max-image-preview:large","max-video-preview":"max-video-preview:-1"},"canonical":"https:\/\/beiyutitanium.com\/de\/titanium-seawater-velocity-erosion-limits\/","og_locale":"de_DE","og_type":"article","og_title":"Titanium Seawater Velocity and Erosion Limits: The Published Data | Beiyu","og_description":"Published erosion rates for titanium in seawater at 25 and 120 ft\/sec, with suspended solids, and 500-hour crevice results by grade. Test conditions stated, failure boundaries included.","og_url":"https:\/\/beiyutitanium.com\/de\/titanium-seawater-velocity-erosion-limits\/","og_site_name":"Beiyu Titanium","article_published_time":"2026-09-02T14:50:00+00:00","article_modified_time":"2026-09-02T15:15:52+00:00","og_image":[{"width":1200,"height":999,"url":"https:\/\/beiyutitanium.com\/wp-content\/uploads\/2026\/06\/grade-12-titanium-weld-neck-flange-astm-b381-asme-b16-5-scaled.jpg","type":"image\/jpeg"}],"author":"Penn Ma","twitter_card":"summary_large_image","twitter_misc":{"Written by":"Penn Ma","Est. reading time":"9 minutes"},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"Article","@id":"https:\/\/beiyutitanium.com\/titanium-seawater-velocity-erosion-limits\/#article","isPartOf":{"@id":"https:\/\/beiyutitanium.com\/titanium-seawater-velocity-erosion-limits\/"},"author":{"name":"Penn Ma","@id":"https:\/\/beiyutitanium.com\/#\/schema\/person\/3560db17cf08813edf34f012735b971b"},"headline":"Titanium in Seawater: What the Velocity and Erosion Data Actually Show","datePublished":"2026-09-02T14:50:00+00:00","dateModified":"2026-09-02T15:15:52+00:00","mainEntityOfPage":{"@id":"https:\/\/beiyutitanium.com\/titanium-seawater-velocity-erosion-limits\/"},"wordCount":1884,"publisher":{"@id":"https:\/\/beiyutitanium.com\/#organization"},"articleSection":["News","Technical Guides"],"inLanguage":"de-DE"},{"@type":"WebPage","@id":"https:\/\/beiyutitanium.com\/titanium-seawater-velocity-erosion-limits\/","url":"https:\/\/beiyutitanium.com\/titanium-seawater-velocity-erosion-limits\/","name":"Grenzwerte f\u00fcr Titan im Meerwasser bei Str\u00f6mungsgeschwindigkeit und Erosion: Die ver\u00f6ffentlichten Daten | Beiyu","isPartOf":{"@id":"https:\/\/beiyutitanium.com\/#website"},"datePublished":"2026-09-02T14:50:00+00:00","dateModified":"2026-09-02T15:15:52+00:00","description":"Ver\u00f6ffentlichte Erosionsraten f\u00fcr Titan in Meerwasser bei 25 und 120 ft\/sec, mit Schwebstoffen, sowie 500-Stunden-Spaltkorrosionsergebnisse nach G\u00fcte. Pr\u00fcfbedingungen angegeben, Versagensgrenzen enthalten.","breadcrumb":{"@id":"https:\/\/beiyutitanium.com\/titanium-seawater-velocity-erosion-limits\/#breadcrumb"},"inLanguage":"de-DE","potentialAction":[{"@type":"ReadAction","target":["https:\/\/beiyutitanium.com\/titanium-seawater-velocity-erosion-limits\/"]}]},{"@type":"BreadcrumbList","@id":"https:\/\/beiyutitanium.com\/titanium-seawater-velocity-erosion-limits\/#breadcrumb","itemListElement":[{"@type":"ListItem","position":1,"name":"Home","item":"https:\/\/beiyutitanium.com\/"},{"@type":"ListItem","position":2,"name":"Titanium in Seawater: What the Velocity and Erosion Data Actually Show"}]},{"@type":"WebSite","@id":"https:\/\/beiyutitanium.com\/#website","url":"https:\/\/beiyutitanium.com\/","name":"Beiyu Titanium","description":"Zertifizierte Titanwerkstoffe und kundenspezifische Komponenten f\u00fcr Anwendungen in Luft- und Raumfahrt, Medizin, Chemie und Industrie.","publisher":{"@id":"https:\/\/beiyutitanium.com\/#organization"},"potentialAction":[{"@type":"SearchAction","target":{"@type":"EntryPoint","urlTemplate":"https:\/\/beiyutitanium.com\/?s={search_term_string}"},"query-input":{"@type":"PropertyValueSpecification","valueRequired":true,"valueName":"search_term_string"}}],"inLanguage":"de-DE"},{"@type":"Organization","@id":"https:\/\/beiyutitanium.com\/#organization","name":"Beiyu Titanium","alternateName":"\u5317\u9a6d\u949b\u4e1a","url":"https:\/\/beiyutitanium.com\/","logo":{"@type":"ImageObject","inLanguage":"de-DE","@id":"https:\/\/beiyutitanium.com\/#\/schema\/logo\/image\/","url":"https:\/\/beiyutitanium.com\/wp-content\/uploads\/2026\/03\/logo4.png","contentUrl":"https:\/\/beiyutitanium.com\/wp-content\/uploads\/2026\/03\/logo4.png","width":429,"height":116,"caption":"Beiyu Titanium"},"image":{"@id":"https:\/\/beiyutitanium.com\/#\/schema\/logo\/image\/"},"sameAs":["https:\/\/www.linkedin.com\/company\/113015050\/","https:\/\/www.youtube.com\/channel\/UC4Rr5qjUmKbbnROzU8zwluQ","https:\/\/www.instagram.com\/beiyutrade\/","https:\/\/www.facebook.com\/people\/Beiyu-Titanium-Group\/61580787646046\/","https:\/\/www.crunchbase.com\/organization\/beiyu-titanium","https:\/\/www.wikidata.org\/wiki\/Q140386451"],"contactPoint":{"@type":"ContactPoint","contactType":"sales","email":"penn@beiyutitanium.com","availableLanguage":["English","Chinese"]},"description":"Beiyu Titanium (Rechtstr\u00e4ger Jiaxing Beiyu New Materials Technology Co., Ltd.) ist ein in China ans\u00e4ssiger Lieferant und Exporteur von ASTM- und AMS-Titanstab, -platte, -blech, -rohr (Tube und Pipe), -schmiedeteilen, -flanschen, -verbindungselementen und kundenspezifisch zerspanten Teilen sowie von Nickel- und Inconel-Legierungen f\u00fcr K\u00e4ufer aus Chemie, Schifffahrt, Medizintechnik und Industrie weltweit. Die Produktion l\u00e4uft \u00fcber Beiyus Titanwerk in Baoji, Shaanxi. Bestellungen erfolgen auf Anfragebasis, mit Werkstoffzeugnissen 3.1 nach EN 10204 und Chargenr\u00fcckverfolgbarkeit auf Anfrage.","areaServed":"Worldwide","knowsAbout":["Titanium","Titanium alloy","Titanium bar","Titanium sheet and plate","Titanium tube and pipe","Titanium forgings","Titanium wire","Titanium anode"],"address":{"@type":"PostalAddress","streetAddress":"Baotai Road Industrial Park, High-tech Development Zone","addressLocality":"Baoji","addressRegion":"Shaanxi","addressCountry":"CN"},"legalName":"Jiaxing Beiyu New Materials Technology Co., Ltd."},{"@type":"Person","@id":"https:\/\/beiyutitanium.com\/#\/schema\/person\/3560db17cf08813edf34f012735b971b","name":"Penn Ma","image":{"@type":"ImageObject","inLanguage":"de-DE","@id":"https:\/\/secure.gravatar.com\/avatar\/0659bdefb633d0d8e567b06d2f8bffac2a369834e53e96c922a06fd8a96f3c72?s=96&d=mm&r=g","url":"https:\/\/secure.gravatar.com\/avatar\/0659bdefb633d0d8e567b06d2f8bffac2a369834e53e96c922a06fd8a96f3c72?s=96&d=mm&r=g","contentUrl":"https:\/\/secure.gravatar.com\/avatar\/0659bdefb633d0d8e567b06d2f8bffac2a369834e53e96c922a06fd8a96f3c72?s=96&d=mm&r=g","caption":"Penn Ma"},"description":"Penn Ma ist die Person, die bei Beiyu Titanium die Anfragen beantwortet. In \u00fcber 15 Jahren Titanexport hat er gelernt, jede Spezifikationszeile selbst zu pr\u00fcfen und Grade, Norm, Abmessungen, Toleranz und Zertifikatsumfang gegen die Werkskapazit\u00e4t abzugleichen, bevor er anbietet, statt Anfragen \u00fcber eine Vertriebsstelle zu leiten. Zur Titanlieferung kam er von der anderen Seite des Gesch\u00e4fts. Bevor er das internationale Gesch\u00e4ft von Beiyu leitete, arbeitete er bei Koch (Koch-Glitsch) und war direkt an der Abwicklung eines petrochemischen SABIC-Projekts in Fujian, China, beteiligt. Diese Arbeit beruhte auf Pr\u00fcf- und Inspektionspl\u00e4nen, Werkstoffzertifizierung und Chargen-R\u00fcckverfolgbarkeit, der Koordination von Fremdabnahmen sowie Projektdokumentation und Dossierkontrolle. Das sind dieselben vier Dinge, an denen ein K\u00e4ufer aus der Prozessindustrie oder ein regulierter K\u00e4ufer einen Titanlieferanten misst, und weil er sie selbst als Kunde durchsetzen musste, werden sie hier als Teil der Lieferung behandelt, nicht als nachtr\u00e4glich erstellte Unterlagen. Seine t\u00e4gliche Arbeit umfasst die Fragen, die diese Website beantworten soll: die Wahl zwischen Reintitan und legierten Titan-Grades f\u00fcr einen korrosiven Einsatz, das Lesen eines Werkstoffzeugnisses gegen die bestellte Norm und das Zuordnen einer K\u00e4uferbezeichnung (ASTM-Grade, UNS, deutsche Werkstoffnummer oder franz\u00f6sischer NF-Code) zu demselben Metall \u00fcber verschiedene M\u00e4rkte hinweg. Beiyu liefert Halbzeuge aus Titan, Nickellegierungen und Refrakt\u00e4rmetallen in Stab, Rundstab, Platte, Rohr, Block, Ring, Coil, Barren, Schmiedeteilen und zerspanten Teilen, mit Dokumentation nach EN 10204 3.1 und Chargennummer-R\u00fcckverfolgbarkeit.","url":"https:\/\/beiyutitanium.com\/de\/author\/penn-ma\/"}]}},"_links":{"self":[{"href":"https:\/\/beiyutitanium.com\/de\/wp-json\/wp\/v2\/posts\/6030","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/beiyutitanium.com\/de\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/beiyutitanium.com\/de\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/beiyutitanium.com\/de\/wp-json\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"https:\/\/beiyutitanium.com\/de\/wp-json\/wp\/v2\/comments?post=6030"}],"version-history":[{"count":1,"href":"https:\/\/beiyutitanium.com\/de\/wp-json\/wp\/v2\/posts\/6030\/revisions"}],"predecessor-version":[{"id":6031,"href":"https:\/\/beiyutitanium.com\/de\/wp-json\/wp\/v2\/posts\/6030\/revisions\/6031"}],"wp:attachment":[{"href":"https:\/\/beiyutitanium.com\/de\/wp-json\/wp\/v2\/media?parent=6030"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/beiyutitanium.com\/de\/wp-json\/wp\/v2\/categories?post=6030"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/beiyutitanium.com\/de\/wp-json\/wp\/v2\/tags?post=6030"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}