No. Pure tungsten is paramagnetic, and a hand magnet will not pick it up. Its magnetic susceptibility is about 6.8 × 10-5, which puts its relative permeability near 1.00007, within the 1.00001 to 1.003 range, near its low end, that a university physics reference gives for ordinary solids and that everyday usage calls “not magnetic”. The answer changes for two products that carry the tungsten name: heavy alloys made with nickel and iron are slightly magnetic, and cemented tungsten carbide usually responds through its cobalt or nickel binder, by an amount that rises with binder content. If a drawing needs a non-magnetic part, the composition and the limit have to be written on the order.

How weak the attraction is, measured
Iron, nickel and cobalt are ferromagnetic: in the annealed pure metals their relative permeability starts at 70 to 150 and rises into the hundreds or thousands. A paramagnetic metal is attracted to a field only very weakly, and the attraction disappears when the field is removed. Tungsten sits in the second group, and so do titanium, molybdenum and tantalum. The values below come from two reference tables that use different units, so they are listed separately rather than compared directly.
| Metal | Behaviour | Molar susceptibility, χm (10-6 cm3/mol, CGS) | Relative permeability |
|---|---|---|---|
| Tungsten | Paramagnetic | +53 | about 1.00007 (calculated: 1 + 6.8 × 10-5) |
| Molybdenum | Paramagnetic | +72 | just above 1 |
| Titanium | Paramagnetic | +151 | just above 1 |
| Tantalum | Paramagnetic | +154 | just above 1 |
| Nickel, 99 % | Ferromagnetic | no value (ferromagnetic) | 110 initial, 600 maximum |
| Iron, 99.8 % | Ferromagnetic | no value (ferromagnetic) | 150 initial, 5000 maximum |
Two things follow from the table. First, tungsten is less paramagnetic per mole than titanium, molybdenum or tantalum, so as a material it is no more of a magnetic concern than they are. Whether a particular part passes still depends on the limit and test method on the order, measured on that part. Second, a magnet test cannot tell pure tungsten from those other metals; it only tells you whether something ferromagnetic is present.
Tungsten heavy alloy: nickel-iron is slightly magnetic, nickel-copper is not
Counterweights, balance weights and radiation shielding are made both from pure tungsten and from tungsten heavy alloy: tungsten grains held together by a nickel-iron or nickel-copper binder. For heavy alloy, the binder decides the magnetic answer. Heavy alloy producers’ data sheets list nickel-iron compositions as slightly magnetic and nickel-copper compositions as non-magnetic:
| Composition (weight %) | Binder | Magnetic response listed by producers |
|---|---|---|
| 90W-7Ni-3Fe | Nickel-iron | Slightly magnetic |
| 92.5W-5.25Ni-2.25Fe | Nickel-iron | Slightly magnetic |
| 95W-3.5Ni-1.5Fe | Nickel-iron | Slightly magnetic |
| 97W-2.1Ni-0.9Fe | Nickel-iron | Slightly magnetic |
| 90W-6Ni-4Cu | Nickel-copper | Nil |
| 95W-3.5Ni-1.5Cu | Nickel-copper | Nil |
ASTM B777, the specification for tungsten-base high-density alloy, says these alloys may contain elements that make them weakly ferromagnetic, and that where freedom from magnetic response is required, it should be specified in the purchase order. It defines non-magnetic material as having a maximum magnetic permeability of 1.05, measured by ASTM A342/A342M, and it states that Class 4 is not available in a non-magnetic grade. So “non-magnetic heavy alloy” is an order requirement with a number attached, not a property that comes with the material name.

Tungsten carbide is a different answer
Cemented tungsten carbide is tungsten carbide particles bonded with a metal binder, usually cobalt and sometimes nickel. The carbide itself is only weakly paramagnetic; the reference table lists tungsten carbide at +10 in the same molar units. The binder is what responds to a magnet. ASTM B886 relies on this: it measures the magnetic saturation of cemented carbide to compare the relative fraction of magnetic binder phase, cobalt, nickel or iron, and that measurement can be used for acceptance of product to specification. A carbide part that pulls toward a magnet is therefore behaving normally, and how strongly it pulls depends on its binder content; a producer’s design guide gives the relative permeability of cobalt-bonded carbide as typically 1.01 to about 12, rising with cobalt content.
Where the answer actually changes a decision
| Situation | Pure tungsten | Heavy alloy, nickel-iron | Heavy alloy, nickel-copper | Cemented carbide |
|---|---|---|---|---|
| Part sits near sensors, magnets or imaging equipment | Candidate | Listed as slightly magnetic; check against the drawing’s permeability limit first | Candidate | Response depends on binder content |
| Hand-magnet check at incoming inspection | No perceptible pull | May show a slight pull | No perceptible pull | Usually a pull, stronger with more binder |
| Order says non-magnetic | State it with the limit and method | Listed by producers as slightly magnetic; the 1.05 maximum by ASTM A342/A342M decides, so state it and confirm before choosing this binder | 1.05 maximum permeability by ASTM A342/A342M, Class 4 excluded | Outside ASTM B777; agree the requirement separately |
A hand magnet sorts the ferromagnetic cases from the rest but cannot confirm a permeability limit, and it will not tell pure tungsten from molybdenum, tantalum or titanium; density or chemistry has to do that.
Common follow-up questions
Is tungsten more magnetic than titanium? No. Both are paramagnetic, and in the same reference table titanium’s molar susceptibility (+151) is about three times tungsten’s (+53). Neither will hold a magnet. The titanium answer, with permeability by grade, is on the is titanium magnetic page; its Grade 5 figure, 1.00005 at a stated field strength, is a measured alloy value and is not directly comparable with the handbook-derived 1.00007 here, though both are within a ten-thousandth of 1.
Is tungsten heavy alloy magnetic? It depends on the binder. Nickel-iron grades are slightly magnetic; nickel-copper grades are listed as non-magnetic. ASTM B777 treats non-magnetic as a purchase-order requirement with a 1.05 maximum permeability.
Is tungsten carbide magnetic? Usually yes, through its cobalt or nickel binder, and the strength of the response rises with binder content. The tungsten carbide phase itself is only weakly paramagnetic.
Does a material certificate confirm that tungsten is non-magnetic? Only if the order asked for it. The certificate reports what the order and the specification require, so a permeability limit and its test method have to be written on the order to appear there.
Specification detail with sources
Tungsten is listed as paramagnetic with a molar magnetic susceptibility of +53 × 10-6 cm3/mol (CGS), against +151 for titanium, +72 for molybdenum, +154 for tantalum and +10 for tungsten carbide, while iron, nickel and cobalt are listed as ferromagnetic (CRC Handbook of Chemistry and Physics, table “Magnetic Susceptibility of the Elements and Inorganic Compounds”). Tungsten’s magnetic susceptibility (relative permeability minus 1, dimensionless) at 20 °C is given as 6.8 × 10-5, and annealed iron (99.8 %), nickel (99 %) and cobalt (99 %) have initial relative permeabilities of 150, 110 and 70 (HyperPhysics, Georgia State University, “Magnetic Properties of Solids” tables). ASTM B777 notes that tungsten-base high-density alloys may be weakly ferromagnetic, states that freedom from magnetic response, where required, should be specified in the purchase order, defines non-magnetic material as a maximum magnetic permeability of 1.05 by ASTM A342/A342M, and excludes Class 4 from the non-magnetic grade (ASTM B777, scope, §1.4). ASTM B886 measures the magnetic saturation of cemented carbide to compare the relative fraction of cobalt, nickel or iron binder phase and allows its use for product acceptance (ASTM B886, §5.1 and §5.2).
The composition-to-response table above restates heavy alloy producers’ published data sheets; the sheets reviewed for this page give a qualitative entry, not a permeability figure, for each grade. The 1.05 maximum in ASTM B777 is the figure an order can cite; a tighter limit has to be written as its own requirement.
Ordering tungsten where the magnetic requirement is real
State the material family first: pure tungsten, or a heavy alloy with its binder named. For heavy alloy, give the ASTM B777 class and write “non-magnetic, maximum permeability 1.05 per ASTM A342/A342M” if the part needs it, remembering that Class 4 cannot be ordered that way. Beiyu Titanium’s tungsten range lists W1 and W2 together with W-Ni-Fe, W-Mo, W-Cu and W-La compositions on the tungsten category page. Of the listed compositions, W1 and W2 are pure tungsten and W-Ni-Fe is the nickel-iron heavy alloy described above as slightly magnetic. Tungsten bar and rod is quoted against the drawing and purchase specification. Send the composition, the magnetic requirement and its test method with the dimensions, and the enquiry is reviewed against them before quotation.